The composition limits describe alloy A-286. The mechanical data apply to solution-treated and aged VAR round bar.
Chemical composition
Values are percentages by mass. A dash means the source value supplies no numerical bound in that column. A producer’s typical value describes its product. Use the purchase specification to establish acceptance limits.
A-286 composition limits, mass % · Mass %| Element | Minimum | Maximum | Source value or rule | Value basis |
|---|
| C | — | 0.08 | ≤0.08 | Maximum limit |
|---|
| Mn | — | 2 | ≤2.00 | Maximum limit |
|---|
| P | — | 0.025 | ≤0.025 | Maximum limit |
|---|
| S | — | 0.025 | ≤0.025 | Maximum limit |
|---|
| Si | — | 1 | ≤1.00 | Maximum limit |
|---|
| Cr | 13.5 | 16 | 13.50–16.00 | Range |
|---|
| Ni | 24 | 27 | 24.00–27.00 | Range |
|---|
| Mo | 1 | 1.5 | 1.00–1.50 | Range |
|---|
| Ti | 1.9 | 2.35 | 1.90–2.35 | Range |
|---|
| V | 0.1 | 0.5 | 0.10–0.50 | Range |
|---|
| Al | — | 0.35 | ≤0.35 | Maximum limit |
|---|
| B | 0.003 | 0.01 | 0.003–0.010 | Range |
|---|
| Fe | — | — | balance | Balance |
|---|
Sources: United Performance Metals, Alloy A286 · Source register
Mechanical properties
Each table identifies the product form, test condition and whether the values are typical or specified limits. Use the ordered standard and delivery condition for acceptance.
The supplier specifies solution treatment at 1800 °F, quenching, aging at 1325 °F for at least 16 h, and air cooling. Hardness is reported as typical.
Comparable designations
Identical means the same designation in another system. Close equivalent means listed as comparable by the cited source, with different limits. Approximate means related but with a material difference. Treat a close or approximate match as “Nearest Commercial Equivalent (Not Identical — Verify Spec)” and confirm the governing requirements before ordering.
Physical and corrosion data
Request a quotation
Send the grade, standard, size and quantity with your request for quotation.
Sources
Cite a grade value. Use the source linked beside its table. Record the standard edition, product form or test condition, value, units and any stated bound. Add the A-286 reference URL for the published context.
- Elgiloy Specialty Metals, A-286 strip data, accessed 22 November 2026. Strip composition, identifiers and properties.
- ATI, A286 alloy technical data sheet, Allvac. Physical properties, melting range.
- United Performance Metals, Alloy A286. A286 Chemical Composition, weight percent.
- Earle M. Jorgensen, Stainless Steels and Super Alloys. Section I, p. 40, A-286 VAR rounds, mechanical properties.
Reference data, not a material certificate. Limits are quoted from the edition named in each table; standards are revised, so check the current edition and your purchase order. Acceptance is decided by the mill test certificate against the standard and edition your order names. Steel Impex India confirms availability per requirement.
Checklist before accepting an alternative
Record the complete grade and standard edition from your order. Use the heat number to match the supplied material to its mill test certificate. Compare the measured results with the limits stated on the order.
Confirm the material family with your supplier. Check how the offered product will behave in your forming, welding and service conditions. Ask for the density of the supplied condition and enter it in the weight calculator. Typical density presets are editable estimates.
For an alternative grade, check product dimensions, processing condition and the intended application with the responsible engineer before ordering. Generic grade names alone are insufficient for substitution.
ASTM catalogue · BIS catalogue · Check values against your order · Standards and sources · Send your requirement and MTC